In Vitro Biocompatibility of Co-Cr Alloys with Different Content of Copper
Xin ZHAO1,2,3,4,Yang CAO1,2,3,Zhun YIN1,2,3,Guangping ZHANG5,Yibin REN6,Desong ZHAN1,2,3,4,*()
1. Department of Prosthetics, School of Stomatology, China Medical University, Shenyang 110002, China
2. Central Laboratory, School of Stomatology, China Medical University, Shenyang 110002, China
3. Liaoning Institute of Dental Research, Shenyang 110002, China
4. Liaoning Province Ord Diseases Translational Medicine Research Center, Shenyang 110002, China
5. Department of Stomatology, Sheng Jing Hospital of China Medical University, Shenyang 110011, China
6. Institute of Metal Research, Chinese Academy of Sciences, Shenyang 110016, China
引用本文:

赵昕,曹阳,印准,张光平,任伊宾,战德松. 不同铜含量钴铬合金的体外生物相容性[J]. 材料研究学报, 2015, 29(8): 627-633.
Xin ZHAO, Yang CAO, Zhun YIN, Guangping ZHANG, Yibin REN, Desong ZHAN. In Vitro Biocompatibility of Co-Cr Alloys with Different Content of Copper[J]. Chinese Journal of Materials Research, 2015, 29(8): 627-633.

全文: PDF(5248 KB)   HTML
摘要: 

用CCK-8法和Annexin-V/PI双标记法研究了不同铜含量(质量分数, 下同)的钴铬合金和钴铬合金的体外生物相容性(包括L929细胞增殖和凋亡)的影响。结果表明, 4种合金的体外生物相容性按含1%铜的钴铬合金、含2%铜的钴铬合金、钴铬合金、含3%铜的钴铬合金的顺序递减; 其细胞毒性等级都为1级, 具有良好的体外生物相容性。

关键词 金属材料含铜钴铬合金细胞毒性细胞增殖细胞凋亡生物相容性    
Abstract

The in vitro biocompatibility (i.e. the cell proliferation and apoptosis of L929 cells) of 4 cast dental alloys (CoCrMo+1%Cu, CoCrMo+2%Cu, CoCrMo+3%Cu and CoCrMo) were evaluated by CCK-8 and Annexing-V/PI double marking methods to provide a biology reference in the clinical application of prosthodontics. Results show that the in vitro biocompatibility of 4 alloys decreases according to following sequence: CoCrMo+1%Cu, CoCrMo+2%Cu, CoCrMo and CoCrMo+3%Cu. However, the cytotoxicity grades of the 4 alloys are all ranked in level one, implying they are good enough in vitro biocompatibility.

Key wordsmetallic materials    copper-cobalt-chromium alloy    cytotoxicity    cellproliferation    apoptosis    biocompatibility
收稿日期: 2014-12-31     
No. Materials Main composition
A CoCrMo Co 56.04,Cr 22.83,Mo 1.09
B CoCrMo+1%Cu Co 60.21,Cr 26.62,Mo 6.15,Cu 1.24
C CoCrMo+2%Cu Co 64.65,Cr 27.25,Mo 6.00,Cu 2.10
D CoCrMo+3%Cu Co 62.23,Cr 28.62,Mo 6.27,Cu 2.88
表1  实验用合金分组及其主要成分
图1  各组细胞在各时间点的细胞形态
Group 24 h 48 h 72 h
RGR Level RGR Level RGR Level
CoCrMo 82.40% 1 81.04% 1 84.21% 1
CoCrMo+1%Cu 95.09% 1 95.30% 1 96.74% 1
CoCrMo+2%Cu 86.41% 1 91.09% 1 94.88% 1
CoCrMo+3%Cu 80.93% 1 80.04% 1 82.40% 1
Positive control group 37.15% 3 37.65% 3 37.09% 3
表2  4组合金对L929细胞的相对增殖率和细胞毒性等级
Groups 24 h 48 h 72 h
CoCrMo 0.4199 ± 0.0744 0.6862±0.0688 1.3627±0.0808
CoCrMo+1%Cu 0.4654 ± 0.0570 0.7850±0.1584 1.5469±0.0987b
CoCrMo+2%Cu 0.4343±0.0513 0.7558±0.0476 1.5196±0.1596
CoCrMo+3%Cu 0.4147±0.0379 0.6793±0.0396a 1.3360±0.0447a,c
Negative control group 0.4830±0.0840 0.8175±0.0784 1.5947±0.1676
Positive control group 0.2578±0.0318a,b 0.3856±0.0759a,b 0.6701±0.0775a,b
表3  不同培养时间点各组的吸光度值( x ? ±s , n=6)
图3  各组细胞培养48 h后流式细胞仪检测早期凋亡率
Groups Early apoptosis rate P
CoCrMo 4.10±0.45 0.003a
CoCrMo+1%Cu 2.80±0.66 0.385a 0.027b
CoCrMo+2%Cu 3.33±0.38 0.039a 0.038b
CoCrMo+3%Cu 4.37±0.26 0.005a
0.427b
Negative control group 2.36±0.40 -
表4  各组细胞48 h早期凋亡率( x ? ±s , n=3)
1 MA Qian,WU Fengming, Study of released metal ions of three kinds of dental casting alloys, Stomatology, 31(1), 33(2011)
1 (马 骞, 吴凤鸣, 3种烤瓷铸造合金的离子析出研究, 口腔医学, 31(1), 33(2011))
2 LU Dongmin,XIE Guangping, SHENG Meichun, WANG Zhonghua, The apoptosis of L-929 cells induced by four kinds of dental ceramic alloys, Shanxi Medical Journal, 38(2), 131(2009)
2 (卢东民, 谢广平, 盛美春, 王忠华, 4种烤瓷合金材料诱导L929细胞凋亡的研究, 陕西医学杂志, 38(2), 131(2009))
3 LI Hongyang,ZHONG Lifang, LIU Bing, CAI Hongdan, Influences of cobalt-chromium alloy versus silver-palladium alloy porcelain crown on periodontal tissues, Journal of Clinical Rehabilitative Tissue Engineering Research, 17(21), 3893(2013)
3 (李洪洋, 钟丽芳, 刘 兵, 蔡鸿丹, 钴铬合金及银钯合金烤瓷冠对牙周组织的影响, 中国组织工程研究, 17(21), 3893(2013))
4 XU Fang,Quantitative Changes of Microflora on Stress-bearing Areas and Satisfaction Relating to Different Metal Base of Partial Denture, Master Thesis(Wenzhou, East China University of Science and Technology, 2013)
4 (徐 芳, 不同金属材料义齿基托对承托区口腔黏膜微生物、义齿性口炎影响, 硕士学位论文(温州, 华东理工大学, 2013))
5 H. Chai, L. Guo, X. Wang, Y. Fu, J. Guan, L. Tan, L. Ren, K. Yang,Antibacterial effect of 317L stainless steel contained copper in prevention of implant-related infection in vitro and in vivo, J. Mater. Sci. Mater. Med., 22(11), 2525(2011)
6 KANG Xiaoyan,WEI Fang, ZHAN Desong, Cytotoxicity evaluation of the nickel-chromium ceramic alloy made by oneself, Chinese Journal of Practical Stomatology, 1(8), 476(2008)
6 (康晓燕, 卫 芳, 战德松, 自制含钛镍铬烤瓷合金的细胞毒性评价, 中国实用口腔科杂志, 1(8), 476(2008))
7 T. Kishimoto, Y. Fukuzawa, M. Abe, M. Hashimoto, M. Ohno, M. Tada,Injury to cultured human vascular endothelial cells by copper (CuSO4) , Nihon. Eiseigaku. Zasshi., 47(5), 965(1992)
8 YU Tianhao,ZHANG Ning, ZHAN Desong, Evaluation of biocompatibilities of three dental alloys by flow cytometry, Chin. J. Mater. Res., 27(6), 652(2013)
8 (毓天昊, 张 宁, 战德松, 使用流式细胞仪评价3种牙科合金材料的生物相容性, 材料研究学报, 27(6), 652(2013))
9 L. C. Rusu, C. M. Bortun, G. Tanasie, A. C. Podariu, F. Baderca, C. Solovan, L. Ardelean,The cytotoxicity of dental alloys studied on cell culture, Rom. J. Morphol. Embryol., 55(1), 111(2014)
10 M. ?oli?, R. Rudolf, D. Stamenkovi?, I. An?el, D. Vu?evi?, M. Jenko, V. Lazi?, G. Lojen,Relationship between microstructure, cytotoxicity and corrosion properties of a Cu-Al-Ni shape memory alloy, Acta Biomater., 6(1), 308(2010)
11 R. K. Sani, B. M. Peyton, L. T. Brown,Copper-induced inhibition of growth of Desulfovibriodesulfuricans G20: assessment of its toxicity and correlation with those of zinc and lead , Appl. Environ. Microbiol., 67(10), 4765(2001)
12 H. Xie, Y. J. Kang,Role of copper in angiogenesis and its medicinal implications, Curr. Med. Chem., 16(10), 1304(2009)
13 S. Li, M. Wang, X. Chen, S. Li, J. L. Ling, H. Xie,Inhibition of osteogenic differentiation of mesenchymal stem cells by copper supplementation , Cell Proliferat., 47(1), 81(2014)
14 C. A. Grillo, M. L. Morales, M. V. Mirifico, L. D. M. M. Fernandez,Synergistic cytotoxic effects of ions released by zinc-aluminum bronze and the metallic salts on osteoblastic cells, J. Biomed. Mater. Res. A, 101(7), 2129(2013)
15 JIANG Lizhu,Induction of apoptosis in L929 murine fibroblasts in response to stainless steel which caps the magnetic attacbanent, Master Thesis(Shenyang, China Medical University, 2004)
15 (蒋立柱,磁性附着体外包裹不锈钢材料对小鼠成纤维细胞L-929凋亡的影响, 硕士学位论文(沈阳, 中国医科大学, 2004))
16 T. Keswani, S. Mitra, A. Bhattacharyya: Copper-induced immunotoxicity involves cell cycle arrest cell death in the liver, Environ. Toxicol., (2013)
17 S. Mitra, T. Keswani, M. Dey, S. Bhattacharya, S. Sarkar, S. Goswami, N. Ghosh, A. Dutta, A. Bhattacharyya: Copper-induced immunotoxicity involves cell cycle arrest cell death in the spleen thymus, Toxicology, 293(1-3), 78(2012)
18 R. G. Contreras, J. R. Vilchis, H. Sakagami, Y. Nakamura, Y. Nakamura, Y. Hibino, H. Nakajima, J. Shimada,Type of cell death induced by seven metals in cultured mouse osteoblastic cells, In Vivo, 24(4), 507(2010)
[1] 毛建军, 富童, 潘虎成, 滕常青, 张伟, 谢东升, 吴璐. AlNbMoZrB系难熔高熵合金的Kr离子辐照损伤行为[J]. 材料研究学报, 2023, 37(9): 641-648.
[2] 宋莉芳, 闫佳豪, 张佃康, 薛程, 夏慧芸, 牛艳辉. 碱金属掺杂MIL125CO2 吸附性能[J]. 材料研究学报, 2023, 37(9): 649-654.
[3] 赵政翔, 廖露海, 徐芳泓, 张威, 李静媛. 超级奥氏体不锈钢24Cr-22Ni-7Mo-0.4N的热变形行为及其组织演变[J]. 材料研究学报, 2023, 37(9): 655-667.
[4] 邵鸿媚, 崔勇, 徐文迪, 张伟, 申晓毅, 翟玉春. 空心球形AlOOH的无模板水热制备和吸附性能[J]. 材料研究学报, 2023, 37(9): 675-684.
[5] 幸定琴, 涂坚, 罗森, 周志明. C含量对VCoNi中熵合金微观组织和性能的影响[J]. 材料研究学报, 2023, 37(9): 685-696.
[6] 欧阳康昕, 周达, 杨宇帆, 张磊. LPSOMg-Y-Er-Ni合金的组织和拉伸性能[J]. 材料研究学报, 2023, 37(9): 697-705.
[7] 徐利君, 郑策, 冯小辉, 黄秋燕, 李应举, 杨院生. 定向再结晶对热轧态Cu71Al18Mn11合金的组织和超弹性性能的影响[J]. 材料研究学报, 2023, 37(8): 571-580.
[8] 熊诗琪, 刘恩泽, 谭政, 宁礼奎, 佟健, 郑志, 李海英. 固溶处理对一种低偏析高温合金组织的影响[J]. 材料研究学报, 2023, 37(8): 603-613.
[9] 刘继浩, 迟宏宵, 武会宾, 马党参, 周健, 徐辉霞. 喷射成形M3高速钢热处理过程中组织的演变和硬度偏低问题[J]. 材料研究学报, 2023, 37(8): 625-632.
[10] 由宝栋, 朱明伟, 杨鹏举, 何杰. 合金相分离制备多孔金属材料的研究进展[J]. 材料研究学报, 2023, 37(8): 561-570.
[11] 任富彦, 欧阳二明. g-C3N4 改性Bi2O3 对盐酸四环素的光催化降解[J]. 材料研究学报, 2023, 37(8): 633-640.
[12] 王昊, 崔君军, 赵明久. 镍基高温合金GH3536带箔材的再结晶与晶粒长大行为[J]. 材料研究学报, 2023, 37(7): 535-542.
[13] 刘明珠, 樊娆, 张萧宇, 马泽元, 梁城洋, 曹颖, 耿仕通, 李玲. SnO2 作散射层的光阳极膜厚对量子点染料敏化太阳能电池光电性能的影响[J]. 材料研究学报, 2023, 37(7): 554-560.
[14] 秦鹤勇, 李振团, 赵光普, 张文云, 张晓敏. 固溶温度对GH4742合金力学性能及γ' 相的影响[J]. 材料研究学报, 2023, 37(7): 502-510.
[15] 刘天福, 张滨, 张均锋, 徐强, 宋竹满, 张广平. 缺口应力集中系数对TC4 ELI合金低周疲劳性能的影响[J]. 材料研究学报, 2023, 37(7): 511-522.