Please wait a minute...
Chinese Journal of Materials Research  2015, Vol. 29 Issue (6): 401-409    DOI: 10.11901/1005.3093.2014.401
Current Issue | Archive | Adv Search |
Short-term Oxidation Behavior of Domestic Forged and Solution Annealed 316LN Stainless Steel in High Temperature Pressurized Water
Yueling GUO1,2,En-Hou HAN2,1,**(),Jianqiu WANG2
1. National Center for Materials Service Safety, University of Science and Technology Beijing,
Beijing 100083, China
2. Key Laboratory of Nuclear Materials and Safety Assessment, Institute of Metal Research, Chinese Academy of Sciences, Shenyang 110016, China
Cite this article: 

Yueling GUO,En-Hou HAN,Jianqiu WANG. Short-term Oxidation Behavior of Domestic Forged and Solution Annealed 316LN Stainless Steel in High Temperature Pressurized Water. Chinese Journal of Materials Research, 2015, 29(6): 401-409.

Download:  HTML  PDF(5563KB) 
Export:  BibTeX | EndNote (RIS)      
Abstract  

Effect of forging on the average grain size, residue strain and grain orientation distribution of nuclear grade 316LN stainless steel (316LNss) was studied by means of electron back scattering diffraction (EBSD). The morphology and chemical composition of the oxide films formed on the as-received 316LNss as well as the forged and solution annealed 316LNss after immersion in borated and lithiated high temperature pressurized water at 300 oC for 190 h were also investigated. The results show that the average grain size was reduced and the residual strain was eliminated by forging and followed solution annealing. There were no obvious textures in the forged and solution annealed 316LNss. A two-layered oxide film grew on 316LNss after immersion in high temperature pressurized water. The outer layer composes of hydroxides and Fe-enriched spinal oxides and the inner layer composes of Cr-enriched spinal oxides. The forged and solution annealed 316LNss exhibited a lower oxidation rate rather than the as received ones due to the formation of a thinner and more Cr-enriched oxide film. The oxidation mechanism was also discussed.

Key words:  material failure and protection      316LN stainless steel      oxide film      high temperature pressurized water      forging      corrosion      nuclear power     
Received:  11 August 2014     
Fund: *Supported by National Science and Technology Major Project No. 2011ZX06004-009.

URL: 

https://www.cjmr.org/EN/10.11901/1005.3093.2014.401     OR     https://www.cjmr.org/EN/Y2015/V29/I6/401

C Cr Ni Mo N Mn Si Cu S P Fe
0.010 17.07 12.87 2.21 0.12 1.35 0.26 0.06 0.003 0.023 Bal
Table 1  Chemical compositions of 316LNss (%, mass fraction)
Element Detailed XPS spectra(± 0.2 eV)
Fe 2p2/3 Peak Fe0 Fe2+ Fe3+
EB/eV 707.0 709.3 711
Ni 2p2/3 Peak Ni0 Ni(II) Ni(OH)2 Ni0Sat Ni(II)Sat
EB/eV 852.6 854.9 856.1 858.5 861.6
Cr 2p2/3 Peak Cr(III) CrOOH Cr0
EB/eV 576.6 577.4 574.1
O 1s Peak O2- OH-
EB/eV 530.3 531.5
Table 2  Binding energies of XPS-peaks of standards[22]
Fig.1  Microstructure and grain orientations of 316LNss, (a) GAM mapping of the as-received 316LNss, (b) PF mapping of the as-received 316LNss, (c) GAM mapping of the forged and solution anneal treated 316LNss, (d) PF mapping of the forged and solution anneal treated 316LNss
Fig.2  SEM images of oxide films grown on 316LNss after immersion in high temperature pressurized water for 190 h, (a) as-received, (b) forged and solution anneal treated
Fig.3  XRD spectra of oxide film grown on 316LNss after immersion in high temperature pressurized water for 190 h
Fig.4  Composition profiles of the oxide films grown on 316LNss after immersion in high temperature pressurized water for 190 h, (a) as-received, (b) forged and solution anneal treated
Fig.5  Normalized content (atomic fraction) of Fe, Ni, Cr contained in the oxide films of the as-received 316LNss and the forged and solution anneal treated 316LNss
Fig.6  Detailed XPS spectra of Cr 2p2/3 in the oxide film grown on 316LNss after immersion in high temperature pressurized water for 190 h, (a) as-received, (b) forged and solution anneal treated
Fig.7  Detailed XPS spectra of Ni 2p2/3 in the oxide film grown on 316LNss after immersion in high temperature pressurized water for 190 h, (a) as-received, (b) forged and solution anneal treated
Fig.8  Detailed XPS spectra of Fe 2p2/3 in the oxide films grown on 316LNss after immersion in high temperature pressurized water for 190 h, (a) as-received, (b) forged and solution anneal treated
Fig.9  Detailed XPS spectra of O 1s in the oxide film grown on 316LNss after immersion in high temperature pressurized water for 190 h, (a) as-received; (b) forged and solution anneal treated
Oxide O Cr Fe Ni
As-received A1 35.66 10.36 44.60 09.38
A2 35.51 09.42 46.63 08.44
Forged and solution anneal treated B1 34.71 10.31 45.55 09.43
B2 35.53 11.07 43.87 09.53
Table 3  SEM-EDS results of the oxides grown on 316LNss after immersion in high temperature pressurized water for 190 h (%, atomic fraction)
Fig.10  Layer model of the oxide film formed on 316LNss in high temperature pressurized water
1 J. Panter, B. Viguier, J. M. Cloué, M. Foucault, P. Combrade, E. Andrieu,Influence of oxide films on primary water stress corrosion cracking initiation of alloy 600, Journal of Nuclear Materials, 348(1), 213(2006)
2 S. Wang, T. Shoji, N. Kawaguchi,Initiation of environmentally assisted cracking in high-temperature water, Corrosion, 61(2), 137(2005)
3 S. M. Bruemmer, L. E. Thomas, Insights into stress-corrosion cracking mechanisms from high-resolution measurements of crack-tip structures and compositions in: MRS Proceedings, edited by J. K. Gibson, S. K. McCall, E. D. Bauer, L. Soderholm, T. Fanghaenel, R. Devanathan, A. Misra, C. Trautmann, B. D. Wirth (UK, Cambridge Univ Press, 2010) P. 1264-BB01-09
4 D. D. MacDonald, M. Urquidi-MacDonald,A coupled environment model for stress corrosion cracking in sensitized type 304 stainless steel in LWR environments, Corrosion Science, 32(1), 51(1991)
5 R. B. Rebak, Z. Szklarska-Smialowska,The mechanism of stress corrosion cracking of alloy 600 in high temperature water, Corrosion Science, 38(6), 971(1996)
6 M. Bojinov, A. Galtayries, P. Kinnunen, A. Machet, P. Marcus,Estimation of the parameters of oxide film growth on nickel-based alloys in high-temperature water electrolytes, Electrochimica Acta, 52(26), 7475(2007)
7 X. Liu, X. Wu, E. -H Han,Effect of Zn injection on established surface oxide films on 316L stainless steel in borated and lithiated high temperature water, Corrosion Science, 65, 136(2012)
8 X. Liu, X. Wu, E. -H Han,Electrochemical and surface analytical investigation of the effects of Zn concentrations on characteristics of oxide films on 304 stainless steel in borated and lithiated high temperature water, Electrochimica Acta, 108, 554(2013)
9 Y. Soma, C. Kato, M. Yamamoto,Multilayered surface oxides within crevices of Type 316L stainless steels in high-temperature pure water, Corrosion, 70(4), 366(2014)
10 D. Féron,E. Herms , B. Tanguy, Behavior of stainless steels in pressurized water reactor primary circuits, Journal of Nuclear Materials, 427(1), 364(2012)
11 X. Liu, E. -H HanX. Wu,Effects of pH value on characteristics of oxide films on 316L stainless steel in Zn-injected borated and lithiated high temperature water, Corrosion Science, 78, 200(2014)
12 W. Kuang, X. E. -H Han Wu. Influence of dissolved oxygen concentration on the oxide film formed on Alloy 690 in high temperature water, Corrosion Science, 69, 197(2013)
13 J. Kim, D. Kim, S. Suwas, E. Fleury, K. Yi,Grain-size effects on the high-temperature oxidation of modified 304 austenitic stainless steel, Oxidation of Metals, 79(3), 239(2013)
14 L. Tan, K. Sridharan, T. R. Allen,The effect of grain boundary engineering on the oxidation behavior of Incoloy alloy 800H in supercritical water, Journal of Nuclear Materials, 348(3), 263(2006)
15 S. Cissé, L. Laffont, M. Lafont, B. Tanguy, E. Andrieu,Influence of localized plasticity on oxidation behaviour of austenitic stainless steels under primary water reactor, Journal of Nuclear Materials, 433(1), 319(2013)
16 S. Lozano-Perez, K. Kruska, I. Iyengar, T. Terachi, T. Yamada,The role of cold work and applied stress on surface oxidation of 304 stainless steel, Corrosion Science, 56, 78(2012)
17 J. Hou, T. Shoji, Z. P. Lu, Q. J. Peng, J. Q. Wang, E. -H. Han, W. Ke,Residual strain measurement and grain boundary characterization in the heat-affected zone of a weld joint between Alloy 690TT and Alloy 52, Journal of Nuclear Materials, 397(1), 109(2010)
18 Q. J. Peng, J. Hou, T. Yonezawa, T. Shoji, Z. M. Zhang, F. Huang, E. -H. Han, W. Ke,Environmentally assisted crack growth in one-dimensionally cold worked Alloy 690TT in primary water, Corrosion Science, 57, 81(2012)
19 T. Sakai, A. Belyakov, R. Kaibyshev, H. Miura, J. J. Jonas,Dynamic and post-dynamic recrystallization under hot, cold and severe plastic deformation conditions, Progress in Materials Science, 60, 130(2014)
20 Y. Cao, H. Di, J. Zhang, J. Zhang, T. Ma, R. D. K. Misra,An electron backscattered diffraction study on the dynamic recrystallization behavior of a nickel-chromium alloy (800H) during hot deformation, Materials Science and Engineering A, 585, 71(2013)
21 ZHANG Litao,WANG Jianqiu, Stress corrosion crack propagation behavior of domestic forged nuclear grade 316L stainless steel in high temperature and high pressure water, Acta Metallurgica Sinica, 49(08), 911(2013)
21 (张利涛, 王俭秋, 国产锻造态核级管材316L不锈钢在高温高压水中的应力腐蚀裂纹扩展行为, 金属学报, 49(08), 911(2013)
22 J. F. Moulder, F. S. William, E. S. Peter, Handbook of X-ray Photoelectron Spectroscopy (USA, Perkin-Elmer Corporation, 1992) p. 72
23 Z. Zhang, J. Q. Wang, E.-H. Han,Characterization of different surface states and its effects on the oxidation behaviours of Alloy 690TT, Journal of Materials Science and Technology, 28(4), 353(2012)
24 S. Perrin, L. Marchetti, C. Duhamel, M. Sennour, F. Jomard,Influence of irradiation on the oxide film formed on 316?L stainless steel in PWR primary water, Oxidation of Metals, 80(5), 623(2013)
25 X. Liu, X. Wu, E. -H. Han,Effect of Zn injection on established surface oxide films on 316L stainless steel in borated and lithiated high temperature water, Corrosion Science, 65, 136(2012)
26 P. Marcus, J. M. Grimal,The anodic dissolution and passivation of NiCrFe alloys studied by ESCA, Corrosion Science, 33(5), 805(1992)
27 H. Sun, X. Wu, E. -H. Han,Effects of temperature on the oxide film properties of 304 stainless steel in high temperature lithium borate buffer solution, Corrosion Science, 51(12), 2840(2009)
28 B. Stellwag,The mechanism of oxide film formation on austenitic stainless steels in high temperature water, Corrosion Science, 40(2), 337(1998)
29 F. Huang, J. Q. Wang, E. -H. Han, W. Ke,Short-time oxidation of Alloy 690 in high-temperature and high-pressure steam and water, Journal of Materials Science and Technology, 28(6), 562(2012)
30 H. Sun, X. Wu, E. -H. Han, Y. Wei,Effects of pH and dissolved oxygen on electrochemical behavior and oxide films of 304SS in borated and lithiated high temperature water, Corrosion Science, 59, 334(2012)
31 N. K. DasT. Shoji,Early Stage oxidation initiation at different grain boundaries of fcc Fe-Cr binary alloy: a computational chemistry study, Oxidation of Metals, 79(3), 429(2013)
32 V. A. Ignatova, S. Van Dyck, R. Gr?tzschel, W. M?ller,XPS depth profiling of oxide scales of stainless steels formed in high-temperature aqueous conditions, Surface and Interface Analysis, 38(4), 396(2006)
33 X. Liu, X. Wu, E.-H. Han,Influence of Zn injection on characteristics of oxide film on 304 stainless steel in borated and lithiated high temperature water, Corrosion Science, 53(10), 3337(2011)
[1] JIANG Menglei, DAI Binbin, CHEN Liang, LIU Hui, MIN Shiling, YANG Fan, HOU Juan. Effect of Building Dimensions by Selective Laser Melting on Pitting Properties of 304L Stainless Steel[J]. 材料研究学报, 2023, 37(5): 353-361.
[2] ZHANG Shuaijie, WU Qian, CHEN Zhitang, ZHENG Binsong, ZHANG Lei, XU Pian. Effect of Mn on Microstructure and Properties of Mg-Y-Cu Alloy[J]. 材料研究学报, 2023, 37(5): 362-370.
[3] YANG Baolei, LIU Tingguang, SU Xianglin, FAN Yu, QIU Liang, LU Yonghao. Effect of Thermal Aging on Mechanical Properties and Intergranular Corrosion Resistance of 316LN[J]. 材料研究学报, 2023, 37(5): 381-390.
[4] LI Pengyu, LIU Zitong, KANG Shumei, CHEN Shanshan. Effect of Plasma Treatment on Performance of Polybutylene Adipate Coating on Biomedical AZ31 Mg-alloy[J]. 材料研究学报, 2023, 37(4): 271-280.
[5] LIAO Hongyu, JIA Yongxin, SU Ruiming, LI Guanglong, QU Yingdong, LI Rongde. Effect of Retrogression Times on Microstructure and Corrosion Resistance of 2024 Aluminum Alloy[J]. 材料研究学报, 2023, 37(4): 264-270.
[6] CHEN Jie, LI Hongying, ZHOU Wenhao, ZHANG Qingxue, TANG Wei, LIU Dan. Effect of Heat Input on Low Temperature Toughness and Corrosion Resistance of Q1100 Steel Welded Joints[J]. 材料研究学报, 2022, 36(8): 617-627.
[7] CAI Yusheng, HAN Hongzhi, REN Dechun, JI Haibin, LEI Jiafeng. Effect of Chemical Etching Process on Surface Roughness of TC4 Ti-alloy Fabricated by Laser Selective Melting[J]. 材料研究学报, 2022, 36(6): 435-442.
[8] YAN Fuzhao, LI Jing, XIONG Liangyin, LIU Shi. Preparation and Microstructure of FeCr-ODS Ferrite Alloy Fabricated by Oxidation and Powder Forging[J]. 材料研究学报, 2022, 36(6): 461-470.
[9] YANG Liuyang, TAN Zhuowei, LI Tongyue, ZHANG Dalei, XING Shaohua, JU Hong. Dynamic Corrosion Behavior of Pipeline Defects Characterized by WBE and EIS Testing Techniques[J]. 材料研究学报, 2022, 36(5): 381-391.
[10] LI Yufeng, ZHANG Nianfei, LIU Lishuang, ZHAO Tiantian, GAO Wenbo, GAO Xiaohui. Preparation of Phosphorus-containing Graphene and Corrosion Resistance of Composite Coating[J]. 材料研究学报, 2022, 36(12): 933-944.
[11] SONG Jianyu, LI Xiang, WANG Qian, SHEN Longhai, QI Dongli, FENG Yu, CHEN Jianjin. Effect of Magnetic Field Direction on Suede Structure of Alkaline Solution Corroded Polysilicon[J]. 材料研究学报, 2021, 35(9): 682-688.
[12] LI Lingmei, HUANG Huizhen, ZHANG Qinghuan, SHUAI Gewang. Effect of P on Properties of Sn-9Zn-0.1S Lead-Free Solder[J]. 材料研究学报, 2021, 35(8): 615-622.
[13] WANG Gen, LI Xinmei, LU Caibin, WANG Songchen, CHAI Cheng. Preparation and Properties of CoCuFeNiTi High Entropy Alloy Coating[J]. 材料研究学报, 2021, 35(8): 561-571.
[14] TANG Rongmao, LIU Guangming, LIU Yongqiang, SHI Chao, ZHANG Bangyan, TIAN Jihong, GAN Hongyu. Assessment on Corrosion Behavior of Q235 Steel in a Simulated Concrete Pore Liquid Containing Chloride by Electrochemical Noise[J]. 材料研究学报, 2021, 35(7): 526-534.
[15] YANG Xiaogang, CUI Shihong, LI Bin, WANG Chuanjie, HAN Jiejia. Preparation and Corrosion Resistance of Graphene/Acetic Acid Doped Polyaniline[J]. 材料研究学报, 2021, 35(5): 357-363.