Effect of Cu Addition on Microstructure, Mechanical Property and Texture Evolution of Extrusion-shearing ZK60 Mg-alloy
Shuai DAI1,2,Feng WANG1,2(),Zhi WANG1,2,Zheng LIU1,2,Pingli MAO1,2
1. School of Materials Science and Engineering, Shenyang University of Technology, Shenyang 110870, China
2. Key Laboratory of Magnesium Alloys and the Processing Technology of Liaoning Province, Shenyang 110870, China
Cite this article: 

Shuai DAI,Feng WANG,Zhi WANG,Zheng LIU,Pingli MAO. Effect of Cu Addition on Microstructure, Mechanical Property and Texture Evolution of Extrusion-shearing ZK60 Mg-alloy. Chinese Journal of Materials Research, 2019, 33(12): 881-891.

Download:  HTML  PDF(8397KB) 
Export:  BibTeX | EndNote (RIS)      
Abstract  

The as-cast Mg-alloys ZK60 and ZK60+1.0Cu (mass fraction, %) were fabricated by permanent mold casting, then, the homogenization heat treatment and two-step extrusion-shearing process were performed for the alloys. The microstructure, phase constitution and mechanical properties of the extrusion-shearing alloys were characterized by means of OM, SEM, EDS, XRD, EBSD, TEM and tensile-compression test at ambient temperature. Results indicated that the ternary MgZnCu phase could be observed in the interiors of α-Mg matrix of the alloy with addition of 1.0Cu. The quantitatively measured average grain size of α-Mg matrix of ZK60+1.0Cu alloy in the forming area was 1.56 μm, which was much less than that of ZK60 alloy (4.68 μm). Furthermore, the sub-grains of 300±45 nm in size were observed around the MgZnCu phase. The ZK60+1.0Cu alloy in the forming area possessed weaker {0001} basal texture while the angle between basal pole and extrusion direction (ED) was changed as compared with ZK60 alloy, resulted in the existence of more dynamic recrystallization (DRX) grains, which was beneficial to {0001}<112ˉ0> basal slip. The tensile and compressive strength of ZK60+1.0Cu alloy in the forming area was obviously higher than that of ZK60 alloy owing to the grain boundary strengthening, and the occurrence of micro-voids near or within the fractured MgZnCu phase mainly accounted for the decrease of tensile elongation.

Key words:  metallic materials      Mg-Zn-Cu-Zr alloy      microstructure      texture evolution      mechanical property     
Received:  29 May 2019     
ZTFLH:  TG146.2  
Fund: National Natural Science Foundation of China(51504153);Liaoning Revitalization Talents Program(XLYC1807021);Youth Project of Liaoning Education Department(LQGD2017032);Innovation Talent Program in Sciences and Technologies for Young and Middle-aged Scientists of Shenyang(RC180111)

URL: 

https://www.cjmr.org/EN/10.11901/1005.3093.2019.281     OR     https://www.cjmr.org/EN/Y2019/V33/I12/881

AlloyNominal compositionActual composition
ZK60Mg-6Zn-0.6ZrMg-5.8Zn-0.61Zr
ZK60+1.0CuMg-6Zn-1.0Cu-0.6ZrMg-5.9Zn-1.1Cu-0.58Zr
Table 1  Chemical compositions of the alloys (mass fraction, %)
Fig.1  The diagram of two-step extrusion-shearing process
Fig.2  OM images of microstructure of extrusion-shearing alloys in extrusion and forming areas (a, b) ZK60 (c, d) ZK60+1.0Cu
Fig.3  SEM images of extrusion-shearing alloys in forming area (a) ZK60, (c) ZK60+1.0Cu, and EDS analyses of (b) MgZn2 and (d) MgZnCu
Fig.4  SEM image and distribution of elements of extrusion-shearing ZK60+1.0Cu alloy in the forming area
Fig.5  XRD spectra of extrusion-shearing ZK60 and ZK60+1.0Cu alloys (a) extrusion area (b) forming area
Fig.6  TEM images of extrusion-shearing ZK60+1.0Cu alloy in the forming area
Fig.7  EBSD orientation and pole figures of extrusion-shearing alloys (a) ZK60, (b) ZK60+1.0Cu
Fig.8  Strain distribution and pole figures of local region of extrusion-shearing alloys (a) ZK60, (b) ZK60+1.0Cu
Fig.9  Distribution of misorientation angle of extrusion-shearing alloys in forming area (a) ZK60, (b) ZK60+1.0Cu
Fig.10  Schmid factor for basal slip of extrusion-shearing alloys in the forming area (a) ZK60, (b) ZK60+1.0Cu
Fig.11  (a) Tensile and (b) compressive stress-strain curves of extrusion-shearing alloys in the forming area
Alloys

UTS

/MPa

TYS

/MPa

CYS

/MPa

δ

/%

CYS

/TYS

ZK60400±10342±7267±527±0.40.78±0.3
ZK60+1.0Cu425±12382±9317±726±0.40.83±0.3
Table 2  Tensile and compression test results of extrusion-shearing alloys in the forming area
Fig.12  SEM images of tensile fracture surface and microstructure of extrusion-shearing alloys in the forming area (a) ZK60 and (b, c) ZK60+1.0Cu, and EDS analysis of (d) MgZnCu and (e) MgZn2
[1] Kulekci M K. Magnesium and its alloys applications in automotive industry [J]. International Journal of Advanced Manufacturing Technology, 2009, 39(9-10): 851
[2] Lin C Y, Bor H Y, Chao C G, et al. Enhanced ductility of the ZA85 magnesium alloy fabricated by equal-channel angular pressing [J]. Journal of Alloys & Compounds, 2013, 556(4): 26
[3] Xiong J J, Chen Z Y, Liu Y, et al. Microstructure and mechanical properties of annealed Mg-0.6wt%Zr sheets by unidirectional and cross rolling [J]. Materials Science & Engineering: A, 2014, 590(1): 60
[4] Bai Y, Cheng W L, Ma S C, et al. Influence of initial microstructure on the strengthening effect of extruded Mg-8Sn-4Zn-2Al alloys [J]. Acta Metallurgica Sinica (English Letters), 2018, 31(5): 487
[5] Zhao Z D, Chen Q, Wang Y B, et al. Microstructures and mechanical properties of AZ91D alloys with Y addition [J]. Materials Science & Engineering A, 2009, 515(1): 152
[6] Wan Y C, Jiang S N, Liu C M, et al. Effect of Nd and Dy on the microstructure and mechanical property of the as extruded Mg-1Zn-0.6Zr alloy [J]. Materials Science and Engineering: A, 2015, 625: 158
[7] Park S H, Kim S H, Kim H S, et al. High-speed indirect extrusion of Mg-Sn-Al-Zn alloy and its influence on microstructure and mechanical properties [J]. Journal of Alloys & Compounds, 2016, 667: 170
[8] Kim S H, Lee J U, Kim Y J, et al. Controlling the microstructure and improving the tensile properties of extruded Mg-Sn-Zn alloy through Al addition [J]. Journal of Alloys and Compounds, 2018, 751: 1
[9] Pan F S, Mao J J, Zhang G, et al. Development of high-strength, low-cost wrought Mg-2.0mass%Zn alloy with high Mn content [J]. Progress in Natural Science: Materials International, 2016, 26(6): 630
[10] Chen X H, Liu L Z, Pan F S, et al. Microstructure, electromagnetic shielding effectiveness and mechanical properties of Mg-Zn-Cu-Zr alloys [J]. Materials Science and Engineering: B, 2015, 197: 67
[11] Figueiredo R B, Langdon T G. The development of superplastic ductilities and microstructural homogeneity in a magnesium ZK60 alloy processed by ECAP [J]. Materials Science & Engineering: A, 2006, 430(1): 151
[12] Wang M Y, Xin R L, Wang B S, et al. Effect of initial texture on dynamic recrystallization of AZ31 Mg alloy during hot rolling [J]. Materials Science & Engineering: A, 2011, 528: 2941
[13] Kim W J, Hong S I, Kim Y S, et al. Texture development and its effect on mechanical properties of an AZ61 Mg alloy fabricated by equal channel angular pressing [J]. Acta Materialia, 2003, 51(11): 3293
[14] Kim W J, An C W, Kim Y S, et al. Mechanical properties and microstructures of an AZ61 Mg Alloy produced by equal channel angular pressing [J]. Scripta Materialia, 2002, 47(1): 39
[15] Dumitru F D, Higuera-Cobos O F, Cabrera J M. ZK60 alloy processed by ECAP: Microstructural, physical and mechanical characterization [J]. Materials Science and Engineering: A, 2014, 594: 32
[16] Zhang D F, Hu H J, Pan F S, et al. Numerical and physical simulation of new SPD method combining extrusion and equal channel angular pressing for AZ31 magnesium alloy [J]. Transactions of Nonferrous Metals Society of China, 2010, 20(3): 478
[17] Dai S, Wang F, Wang Z, et al. The microstructure and mechanical properties of hot-extruded Mg-6Zn-xCu-0.6Zr (x=0, 0.5, 1.0, 1.5) alloys [J]. Hot Working Technology, 2018, 47(3): 28
[17] (代 帅, 王 峰, 王 志等. 热挤压Mg-6Zn-xCu-0.6Zr(x=0,0.5,1.0,1.5)合金的显微组织及力学性 [J]. 热加工工艺, 2018, 47(3): 28)
[18] Shahzad M, Wagner L. Microstructure development during extrusion in a wrought Mg-Zn-Zr alloy [J]. Scripta Materialia, 2009, 60(7): 536
[19] Zhu H M, Sha G, Liu J W, et al. Microstructure and mechanical properties of Mg-6Zn-xCu-0.6Zr (wt.%) alloys [J]. Journal of Alloys and Compounds, 2011, 509: 3526
[20] Buha J, Ohkubo T. Natural aging in Mg-Zn(-Cu) alloys [J]. Metallurgical & Materials Transactions A, 2008, 39(9): 2259
[21] Oh-Ishi K, Mendis C L, Homma T, et al. Bimodally grained microstructure development during hot extrusion of Mg-2.4Zn-0.1Ag-0.1Ca-0.16Zr (at.%) alloys [J]. Acta Materialia, 2009, 57(18): 5593
[22] Wang B S, Shi J J, Ye P, et al. Analysis of {10-12} twinning variants’ selection behavior during multi-directional compression in Mg-3Al-1Zn magnesium alloy[J]. Journal of Materials Science, 2019, 54(13): 9797
[23] Zhao H, Wang L Q, Ren Y P, et al. Microstructure, mechanical properties and corrosion behavior of extruded Mg-Zn-Ag alloys with single-phase structure [J]. Acta Metallurgica Sinica (English Letters), 2018, 31(6): 575
[24] Yin D S, Zhang E L, Zeng S Y. Effect of Zn on mechanical property and corrosion property of extruded Mg-Zn-Mn alloy [J]. Transactions of Nonferrous Metals Society of China, 2008, 18(4): 763
[25] Pan H C, Fu H, Ren Y P, et al. Effect of Cu/Zn on microstructure and mechanical properties of extruded Mg-Sn alloys [J]. Materials Science and Technology, 2016,16: 1743
[26] Xin Y C, Wang M Y, Zeng Z, et al. Tailoring the texture of magnesium alloy by twinning deformation to improve the rolling capability [J]. Scripta Materialia, 2011, 64(10): 986
[27] Koike J, Kobayashi T, Mukai T, et al. The activity of non-basal slip systems and dynamic recovery at room temperature in fine-grained AZ31B magnesium alloys [J]. Acta Materialia, 2003, 51(7): 2055
[28] Yan H, Xu S W, Chen R S, et al. Activation of {10-12} twinning and slip in high ductile Mg-2.0Zn-0.8Gd rolled sheet with non-basal texture during tensile deformation at room temperature [J]. Journal of Alloys & Compounds, 2013, 566(8): 98
[29] Valle J A D, Carreno F, Ruano O A. Influence of texture and grain size on work hardening and ductility in magnesium-based alloys processed by ECAP and rolling [J]. Acta Materialia, 2006, 54(16): 4247
[30] Barnett M R. Twinning and the ductility of magnesium alloys: Part II. “Contraction” twins [J]. Materials Science & Engineering A, 2007, 464(1): 8
[31] Ando D, Koike J, Sutou Y. Relationship between deformation twinning and surface step formation in AZ31 magnesium alloys [J]. Acta Materialia, 2010, 58(13): 4316
[1] PAN Xinyuan, JIANG Jin, REN Yunfei, LIU Li, LI Jinghui, ZHANG Mingya. Microstructure and Property of Ti / Steel Composite Pipe Prepared by Hot Extrusion[J]. 材料研究学报, 2023, 37(9): 713-720.
[2] MAO Jianjun, FU Tong, PAN Hucheng, TENG Changqing, ZHANG Wei, XIE Dongsheng, WU Lu. Kr Ions Irradiation Damage Behavior of AlNbMoZrB Refractory High-entropy Alloy[J]. 材料研究学报, 2023, 37(9): 641-648.
[3] SONG Lifang, YAN Jiahao, ZHANG Diankang, XUE Cheng, XIA Huiyun, NIU Yanhui. Carbon Dioxide Adsorption Capacity of Alkali-metal Cation Dopped MIL125[J]. 材料研究学报, 2023, 37(9): 649-654.
[4] ZHAO Zhengxiang, LIAO Luhai, XU Fanghong, ZHANG Wei, LI Jingyuan. Hot Deformation Behavior and Microstructue Evolution of Super Austenitic Stainless Steel 24Cr-22Ni-7Mo-0.4N[J]. 材料研究学报, 2023, 37(9): 655-667.
[5] SHAO Hongmei, CUI Yong, XU Wendi, ZHANG Wei, SHEN Xiaoyi, ZHAI Yuchun. Template-free Hydrothermal Preparation and Adsorption Capacity of Hollow Spherical AlOOH[J]. 材料研究学报, 2023, 37(9): 675-684.
[6] XING Dingqin, TU Jian, LUO Sen, ZHOU Zhiming. Effect of Different C Contents on Microstructure and Properties of VCoNi Medium-entropy Alloys[J]. 材料研究学报, 2023, 37(9): 685-696.
[7] OUYANG Kangxin, ZHOU Da, YANG Yufan, ZHANG Lei. Microstructure and Tensile Properties of Mg-Y-Er-Ni Alloy with Long Period Stacking Ordered Phases[J]. 材料研究学报, 2023, 37(9): 697-705.
[8] XU Lijun, ZHENG Ce, FENG Xiaohui, HUANG Qiuyan, LI Yingju, YANG Yuansheng. Effects of Directional Recrystallization on Microstructure and Superelastic Property of Hot-rolled Cu71Al18Mn11 Alloy[J]. 材料研究学报, 2023, 37(8): 571-580.
[9] XIONG Shiqi, LIU Enze, TAN Zheng, NING Likui, TONG Jian, ZHENG Zhi, LI Haiying. Effect of Solution Heat Treatment on Microstructure of DZ125L Superalloy with Low Segregation[J]. 材料研究学报, 2023, 37(8): 603-613.
[10] LIU Jihao, CHI Hongxiao, WU Huibin, MA Dangshen, ZHOU Jian, XU Huixia. Heat Treatment Related Microstructure Evolution and Low Hardness Issue of Spray Forming M3 High Speed Steel[J]. 材料研究学报, 2023, 37(8): 625-632.
[11] YOU Baodong, ZHU Mingwei, YANG Pengju, HE Jie. Research Progress in Preparation of Porous Metal Materials by Alloy Phase Separation[J]. 材料研究学报, 2023, 37(8): 561-570.
[12] REN Fuyan, OUYANG Erming. Photocatalytic Degradation of Tetracycline Hydrochloride by g-C3N4 Modified Bi2O3[J]. 材料研究学报, 2023, 37(8): 633-640.
[13] WANG Hao, CUI Junjun, ZHAO Mingjiu. Recrystallization and Grain Growth Behavior for Strip and Foil of Ni-based Superalloy GH3536[J]. 材料研究学报, 2023, 37(7): 535-542.
[14] LIU Mingzhu, FAN Rao, ZHANG Xiaoyu, MA Zeyuan, LIANG Chengyang, CAO Ying, GENG Shitong, LI Ling. Effect of Photoanode Film Thickness of SnO2 as Scattering Layer on the Photovoltaic Performance of Quantum Dot Dye-sensitized Solar Cells[J]. 材料研究学报, 2023, 37(7): 554-560.
[15] QIN Heyong, LI Zhentuan, ZHAO Guangpu, ZHANG Wenyun, ZHANG Xiaomin. Effect of Solution Temperature on Mechanical Properties and γ' Phase of GH4742 Superalloy[J]. 材料研究学报, 2023, 37(7): 502-510.
No Suggested Reading articles found!