GH4065A合金铸态的组织和元素偏析及其均匀化
赵书伟, 孙文儒, 吕文龙, 张伟红, 邱克强

Elements Segregation and Microstructure Homogenization of Cast GH4065A Superalloy
ZHAO Shuwei, SUN Wenru, LV Wenlong, ZHANG Weihong, QIU Keqiang
表3 合金经不同热处理后的残余偏析系数δ值
Table 3 Residual segregation coefficient δ values of the alloy after different heat treatments
No.TreatmentNbTiWMoCoCrAl
0#As-cast3.042.440.611.270.990.991.19
1#1180 oC × 5 h1.551.141.631.271.231.241.41
2#1190 oC × 5 h1.491.271.601.251.221.211.37
3#1200 oC × 5 h1.451.171.491.221.121.121.22
4#1190 oC × 20 h1.561.051.131.111.041.021.12
5#1190 oC × 80 h1.480.981.321.040.980.990.96
6#1110 oC × 20 h + 1160 oC × 20 h + 1180 oC× 60 h1.241.051.211.061.041.021.06
7#1110 oC × 20 h + 1160 oC × 20 h + 1180 oC × 70 h1.421.051.171.121.031.031.11
8#1110 oC × 20 h + 1160 oC × 20 h + 1180 oC × 80 h1.371.051.111.061.031.021.14
9#1110 oC × 20 h + 1160 oC × 20 h + 1190 oC × 60 h1.171.051.261.071.021.031.09
10#1110 oC × 20 h + 1160 oC × 20 h + 1190 oC × 70 h1.261.041.181.041.021.021.06
11#1110 oC × 20 h + 1160 oC × 20 h + 1190 oC × 80 h1.111.041.161.061.041.031.08
12#1110 oC × 20 h + 1160 oC × 20 h + 1200 oC × 60 h1.451.051.231.081.021.031.08
13#1110 oC × 20 h + 1160 oC × 20 h + 1200 oC × 70 h1.351.051.171.041.031.031.13
14#1110 oC × 20 h + 1160 oC × 20 h + 1200 oC × 80 h1.250.981.000.991.000.991.07