SiOC气凝胶/柔性陶瓷纤维复合材料的制备和性能
祝诗洋, 潘栩, 钟业盛, 马晓亮, 高岩, 史丽萍, 李明伟, 赫晓东

Preparation and Properties of SiOC Aerogel/Flexible Ceramic Fiber Composite
ZHU Shiyang, PAN Xu, ZHONG Yesheng, MA Xiaoliang, GAO Yan, SHI Liping, LI Mingwei, HE Xiaodong
表3 SiOC气凝胶/柔性陶瓷纤维复合材料的吸湿率
Table 3 Moisture absorption rate of SiOC aerogel/flexible ceramic fiber composite
Time/d0#1#2#3#4#5#6#7#
01.2450.4890.5130.5530.7690.4640.6810.433
71.2480.4900.5140.5550.7720.4640.6830.433
141.2580.4900.5320.5570.7720.4650.6830.433
211.2620.4920.5320.5580.7740.4660.6840.436
281.3000.4930.5330.5590.7750.4700.6840.439
351.3500.5060.5330.5700.7890.4760.6990.445
Moisture content/%7.7783.3603.7522.9822.5352.5212.5752.697