成核-生长型液-液分相对无铅低温熔剂性能的影响
汪鹏, 卢希龙, 曹春娥, 陈云霞, 沈华荣, 张旭

Influence of Nucleation-growth Liquid-liquid Phase Partition on Properties of Lead-free Low Temperature Frit
WANG Peng, LU Xilong, CAO Chun-e, CHEN Yunxia, SHEN Huarong, ZHANG Xu
表3 非等温热处理对熔剂性能的影响
Table 3 The effect of non-isothermal heat treatment on the performance of frits
CodeR0R1R2R3R4R5
Temperature/℃Water quenching550590630670710
Intial gloss109103108110112106
Gloss after grinding587175816360
Gloss loss/%46.731.130.526.443.743.4
Vickers hardness/MPa495761136158620250655005
wear resistance(750 revolutions)222222