盐雾预腐蚀对HRB400E抗震钢筋超低周疲劳性能的影响
谌理飞, 罗云蓉, 张应迁, 李辉, 李秀兰, 廖文丽

Effect of Pre-corrosion by Salt Spray on Extremely Low Cycle Fatigue Performance of HRB400E Seismic Steel Bar
CHEN Lifei, LUO Yunrong, ZHANG Yingqian, LI Hui, LI Xiulan, LIAO Wenli
表3 ELCF试验结果
Table 3 ELCF test results
Corrosion time/dεa/%εpaεeaNfΔWp/MJ·m-3ΔWe/MJ·m-3ΔWt/MJ·m-3
030.01570.01439821.38.229.5
3.20.0170.0159023.8932.8
3.50.01950.015561289.637.6
40.02370.01634434.310.644.9
3030.01590.01418821829
3.20.01820.01388624.67.632.2
3.50.020.0155827.4936.4
40.02520.01484036.28.744.9
6030.01670.01338420.7727.7
3.20.01840.01367222.77.330
3.50.0210.0145027.37.334.6
40.02550.01453034.18.442.5
9030.0170.0138418.76.7625.46
3.20.01850.01358320.47.2927.69
3.50.0220.0134324.76.7631.46
40.0260.0143131.87.8439.64