P91热轧无缝钢管的TMCP模拟
|
王晓东,郭锋,包喜荣,王宝峰
|
TMCP Simulation for Hot Rolling of P91 Seamless Steel Pipe
|
Xiaodong WANG,Feng GUO,Xirong BAO,Baofeng WANG
|
|
表2 P91钢管TMCP穿孔+PQF连轧+定径模拟工艺参数 |
Table 2 TMCP parameters of piercing, PQF continuous rolling and sizing of P91 pipe |
|
Pass | Equivalent strain | Temperature /℃ | Strain rate /s-1 | Interval time/s |
---|
Heating | - | 1290 | - | - | Piercing | 1.303 | 1250 | 2 | 50 | PQF1 | 0.153 | 1125 | 3 | 0.853 | PQF2 | 0.15 | 1112 | 4 | 1.004 | PQF3 | 0.104 | 1098 | 4 | 0.678 | PQF4 | 0.056 | 1088 | 3 | 0.645 | PQF5 | 0.012 | 1080 | 2 | 50 | Sizing1 | 0.019 | 1040 | 2 | 2 | Sizing 2 | 0.015 | 1036 | 2 | 2 | Sizing 3 | 0.016 | 1025 | 2 | 2 | Sizing 4 | 0.015 | 1018 | 2 | 2 | Sizing 5 | 0.015 | 1004 | 2 | 2 | Sizing 6 | 0.008 | 996 | 2 | 2 | Sizing 7 | 0.008 | 990 | 2 | - |
|
|
|